SPI is the short form of the Society of Plastic Industry, who establish standards for plastic industry and the SPI Plastic Engineering Handbooks is one of the most important reference for engineers.
SPI defines the polishing standard on mold finish and widely applied in US markets. It helps to avoid grey areas and measure the finest of surface in the unit of Rough Average (Ra).

Nowadays, China’s standard is very much in line with SPI. However, there is little help using Ra value in China mold making industry because there is little chance to have precise equipment at site to do the precision measurement. What we needed is a practical guideline to more or less achieve the desired mold finish. Below guideline is widely accepted.
GLOSSY SURFACE, DIAMOND BUFF POLISH
SPI Finish A-1 — Grade #3, 6000 Grit Diamond Buff
SPI Finish A-2 — Grade #6, 3000 Grit Diamond Buff
SPI Finish A-3 — Grade #15, 1200 Grit Diamond Buff
NON-GLOSSY SURFACE, PAPER POLISH
SPI Finish B-1 — 600 Grit Paper
SPI Finish B-2 — 400 Grit Paper
SPI Finish B-3 — 320 Grit Paper
ROUGH SURFACE, STONE POLISH
SPI Finish C-1 — 600 Grit Stone
SPI Finish C-2 — 400 Grit Stone
SPI Finish C-3 — 320 Grit Stone
VERY ROUGH SURFACE, DRY BLASH POLISH
SPI Finish D-1 — 600 Stone Prior to Dry Blast Glass Bead #11
SPI Finish D-2 — 400 Stone Prior to Dry Blast #240 Oxide
SPI Finish D-3 — 320 Stone Prior to Dry Blast #24 Oxide

However, the above guideline falls short because it does not mention what steel should be used. For coarse surface, it may be fine. For demanding high glossy mold finish, the mold steel can be critical and the high glossy cannot be achieved without proper steel.
For molding process, a melt plastic resin will be injected into a steel mold at high pressure and the steel will always face the issue of wear off. To produce a glossy product, the mold has to be significantly hard so that the shiny smooth surface will not be deteriorated quickly and the glossy surface can be remained for a longer period of time. The finer the surface is needed, the harder and the finer the steel is required.
Below is a supplementary guideline regarding steel to be used.
SPI Finish A1 – S136 Hardness at 54HRC
(Generally called “Super High Glossy” in China)
SPI Finish A2 – 718HH or NAK80 Hardness at 40HRC
(Generally called “High Glossy” in China)
SPI Finish A3 – 718H or S136 Hardness 32HRC
(Generally called “Normal Glossy” in China)
It is true that the steel made in China are somehow less consistent than from overseas. Therefore, it is suggested to use imported steel for demanding quality mold or at least use higher grade of steel from China to provide some buffer for the desired mold finish that you need.
Lastly, a high glossy mold finish is not equivalent to a high glossy finished product. It is significantly subject to other factors such as plastic resin used, molding condition and mold design. For example, ABS will provide higher glossy than PP, high temperature molding condition and non-flat surface will help to provide a much glossy finished product.
Superb content, my friend. You are truly a literary genius. This kind of article requires a great mind and a lot of research. I commend you on the hard work you put into this writing.
Youre so cool! I dont suppose Ive read something like this before. So nice to find any individual with some authentic thoughts on this subject. realy thanks for beginning this up. this web site is one thing that’s needed on the web, somebody with a bit of originality. useful job for bringing one thing new to the internet!
Thank you for sharing excellent informations. Your website is very cool. I’m impressed by the details that you have on this blog. It reveals how nicely you perceive this subject. Bookmarked this website page, will come back for more articles. You, my friend, ROCK! I found just the information I already searched everywhere and simply could not come across. What a great site.
I have recently started a web site, the information you provide on this site has helped me tremendously. Thanks for all of your time & work.
Superior article. I commitment certainly due this article with my friends. Thanks fitting for the info.
Whats up! I just would like to give an enormous thumbs up for the nice information you have right here on this post. I can be coming back to your blog for more soon.
hello!,I love your writing so so much! percentage we be in contact more about your article on AOL? I need an expert in this area to resolve my problem. May be that is you! Having a look forward to look you.
Heya i’m for the first time here. I came across this board and I find It really useful & it helped me out a lot. I hope to give something back and help others like you helped me.
Please let me know if you’re looking for a article author for your blog. You have some really good posts and I believe I would be a good asset. If you ever want to take some of the load off, I’d absolutely love to write some content for your blog in exchange for a link back to mine. Please shoot me an e-mail if interested. Cheers!
Just want to say your article is as astounding. The clearness in your post is simply nice and i can assume you’re an expert on this subject. Well with your permission allow me to grab your feed to keep updated with forthcoming post. Thanks a million and please keep up the rewarding work.